I'm new to the site so please take it easy on me, I'd like any information on heat treating and tempering CPM S30V that is .250" thick. I have a gas forge that is rated to 2400 F. As well does anyone have experience with sharpening/grinding this thickness.....Thanks to everyone in advance.
 
I suggest using an oven or paying for heat treating. S30V needs to be foil wrapped, treated at 1900F+ (but not over 2000F) and soaked for at least 15 minutes, a forge is not going to do well for that application.
 
Yes , precise HT is necessary. Grind very close to final dimension before HT. Send it to an experienced HTer.
 