S shqxk Joined Mar 26, 2012 Messages 2,301 Apr 4, 2016 #1 Anyone know heat treat process for this alloy? I heard it can be HT to the mid 40's.
Kohai999 Second Degree Cutter Joined Jul 15, 2003 Messages 12,554 Apr 4, 2016 #2 shqxk said: Anyone know heat treat process for this alloy? I heard it can be HT to the mid 40's. Click to expand... You want to direct this question to Forumite Mecha, who probably knows as much about heat treating titanium as anyone on the boards. Best Regards, STeven Garsson
shqxk said: Anyone know heat treat process for this alloy? I heard it can be HT to the mid 40's. Click to expand... You want to direct this question to Forumite Mecha, who probably knows as much about heat treating titanium as anyone on the boards. Best Regards, STeven Garsson
Alpha Knife Supply Always Innovating Joined Oct 14, 1998 Messages 2,157 Apr 4, 2016 #3 The heat treatment I've used is: 1500°F for 30 min & quench in water. No temper. This will give you about HRC 43-45. Chuck
The heat treatment I've used is: 1500°F for 30 min & quench in water. No temper. This will give you about HRC 43-45. Chuck
Mecha Titanium Bladesmith Knifemaker / Craftsman / Service Provider Joined Dec 27, 2013 Messages 10,151 Apr 4, 2016 #4 ... Last edited: Oct 2, 2021
Mecha Titanium Bladesmith Knifemaker / Craftsman / Service Provider Joined Dec 27, 2013 Messages 10,151 Apr 4, 2016 #5 ... Last edited: Oct 2, 2021
Matthew Gregory Chief Executive in charge of Entertainment Joined Jan 12, 2005 Messages 6,709 Apr 4, 2016 #6 Sam, you rule.
S shqxk Joined Mar 26, 2012 Messages 2,301 Apr 5, 2016 #7 Wow, thanks you Mecha for your very informative response.