on a no BS 52100 heat treat

ok so here we go
i did 1625 soak air cool
1575 soak and air cool
1530 soak and air cool
1510 soak 20 min quench in parks 50 (room temp
cooled blades to room temp and put in LN till the kiln came down to 350 then pulled from LN and tempered 1.5 hours for all razors and one hunting blade
then took them out and bumped the kiln to 400f
the hunter got another hour at 400
razor hardness Rc63 and hunter hardness RC62 i snapped off part of a razor to see the grain and got some crappy pictures i ll update when i think i got "ok" ones
 